Blackbutt, New England

New England blackbutt is a large Australian hardwood from the tablelands of northern New South Wales and southern Queensland used mainly for general construction.

Other Names

New England Ash, New England Peppermint, Eucalyptus campanulata

Botanical Name

Eucalyptus andrewsii

Common Form
Sawn
Species Type

New England blackbutt is a large Australian hardwood that grows in the tablelands and coastal ranges of northern New South Wales and southern Queensland.

Also known as New England ash, it is similar in appearance yet not quite as durable as blackbutt.

The heartwood is pale brown, while the sapwood is much paler in appearance. New England blackbutt has an even texture and generally straight grain. Gum veins are usually present.

New England blackbutt can be stained, painted or polished but there can be issues with painting because of its tendency to surface check. The high extractives of mature wood can cause problems with some adhesives. These extractives can also cause staining on painted surfaces exposed to the weather. Blackbutt machines well but is only fair for steam bending.

A durable hardwood, New England blackbutt is used for general construction applications, flooring and joinery.

 

 

Shrinkage

Very Low Low Medium High Very High
Check mark Check mark Check mark

Tangential : Provides a simplified rating for tangential shrinkage. This is the measure of the percentage reduction in dimension from the unseasoned to 12% moisture content condition.

11.40%

Radial : Radial shrinkage is perpendicular to the growth rings. It is shrinkage in the direction towards the centre of the tree. Measurement is % value

6.10%

Unit Movement Tangential: This is the percentage of dimensional change for each 1% moisture content change between about 3% moisture content and the fibre saturation point for the particular species.

0.36%

Unit Movement Radial: This is the percentage of dimensional change for each 1% moisture content change between about 3% moisture content and the fibre saturation point for the particular species.

0.25%

Strength Group Strength groups are given for unseasoned (S1-S7) and seasoned (SD1-SD8) timber in accordance with AS 2878. S1 and SD1 yield the highest strength and stiffness whereas S7 and SD8 yield the lowest.

Very High

High

Reasonably High

Medium High

Medium

Reasonably Low

Low

Very Low

Unseasoned:

S1

S2

S3

S4

S5

S6

S7

S8

Check mark

Seasoned:

SD1

SD2

SD3

SD4

SD5

SD6

SD7

SD8

Check mark

Stress Grade A stress grade is defined in AS 1720 as the classification of timber for structural purposes by means of either visual or machine grading. The stress grade indicates the basic working stresses and stiffnesses to be used for structural design purposes. Measured in MPa.

Structural
No. 1
Structural
No. 2
Structural
No. 3
Structural
No. 4
Structural
No. 5

Unseasoned:

F17

F14

F11

F8

F7

Seasoned:

F27

F22

F17

F14

F11

Density per Standard Seasoned density is based on moisture content of 12%. Unseasoned density is an approximation as it depends on the moisture content at the time of measurement. Measured kg/m3.

Seasoned:

850kg/m3

Unseasoned:

1150kg/m3

Joint Group The joint group is a classification of the strength of a species in joint design. The values are from 1 (very high strength) to 6 (very low strength).

Very High

High

Reasonably High

Medium

Low

Very Low

Unseasoned:

J1

J2

J3

J4

J5

J6

Check mark

Seasoned:

JD1

JD2

JD3

JD4

JD5

JD6

Check mark

Colour The colour of seasoned heartwood can vary between species and often within a species. The information provided should be used as a general guide only. In most cases, the colour of sapwood is either a lighter shade of the heartwood or a white/cream colour.

  White, yellow, pale straw to light brown Pink to pink brown Light to dark red Brown, chocolate, mottled or streaky
   
Check mark

Mechanical Properties

Modulus of Rupture - Unseasoned: This property is a measure of maximum stress which timber can momentarily sustain when loaded slowly and continuously as a beam. Measured in MPa.

81

Modulus of Rupture - Seasoned: This property is a measure of maximum stress which timber can momentarily sustain when loaded slowly and continuously as a beam. Measured in MPa.

140

Modulus of Elasticity - Unseasoned: This property is of importance in determining the deflection of a beam under load — the greater the stiffness, the less the deflection. Measured in GPa.

12

Modulus of Elasticity - Seasoned: This property is of importance in determining the deflection of a beam under load — the greater the stiffness, the less the deflection. Measured in GPa.

14

Maximum Crushing Strength - Unseasoned:

Also referred to as compression strength. This property measures the ability of the timber to withstand loads applied on the end grain. Measured in MPa.

44

Maximum Crushing Strength - Seasoned: Also referred to as compression strength. This property measures the ability of the timber to withstand loads applied on the end grain. Measured in MPa.

65

Impact - Unseasoned: Provides the Izod value, which is the energy taken in joules (J) to fracture the timber.

18.6

Impact - Seasoned: Provides the Izod value, which is the energy taken in joules (J) to fracture the timber.

20.4

Toughness - Unseasoned: This is a measure of timber’s ability to resist shocks and blows, and is synonymous with impact strength. It is measured in Nm.

Medium - 15 - 24 Nm

Toughness - Seasoned: This is a measure of timber’s ability to resist shocks and blows, and is synonymous with impact strength. It is measured in Nm.

Medium - 15 - 24 Nm

Hardness - Unseasoned: Refers to the Janka hardness test and is a measure of timber’s resistance to indentation.

6.6

Hardness - Seasoned: Refers to the Janka hardness test and is a measure of timber’s resistance to indentation.

9.2

Durability

Low Moderate Reasonably High High
(0 - 5 yrs) (5 - 15 yrs) (15 - 25 yrs) (more than 25 yrs)

In-Ground: Durability is defined as the inherent resistance of a timber species to decay, or to insect or marine borer attack. All references to durability refer to the heartwood only. A scale of low to high (durability class 4 = low; 1 = high) has been adapted for above and in-ground durability.

Check mark
(0 - 7 yrs) (7 - 15 yrs) (15 - 40 yrs) (More than 40 yrs)

Above ground: Durability is defined as the inherent resistance of a timber species to decay, or to insect or marine borer attack. All references to durability refer to the heartwood only. A scale of low to high (durability class 4 = low; 1 = high) has been adapted for above and in-ground durability.

Check mark
(0 - 20 yrs, usually < 5) (21 - 40 yrs) (41 - 64 yrs) (More than 60 yrs)

Marine Borer Resistance: Indicates whether a species is resistant (R) or not resistant (NR) to marine borer attack.

Check mark

Lyctid Borer Susceptibility: Indicates whether a species is susceptible (S) or not susceptible (NS) to lyctid borer attack.

Susceptible

Lyctid Borer Susceptibility - Other:

Termite Resistance: Indicates whether a species is resistant (R) or not resistant (NR) to termites.

Resistant

Fire Properties

0 1 2 3 4 5 6 7 8 9 10

EFH Spread-of-Flame Index: This is a material's propensity to burn rapidly and spread flames based on a scale of 0 to 10 where 0 means that the materials will not cause flames to reach the ceiling and 10 indicates that the material could be expected to cause flames to reach the ceiling of a room within 10 seconds of ignition.

EFH Smoke-Developed Index:This is a measure of the concentration (measured by optical density) of smoke a material emits as it burns. It is based on an arbitrary scale of 0 to 10. The higher the index, the greater the hazard from smoke is likely to be.

Critical Radiance Flux - Lower: This measures the radiant (heat) energy required to sustain burning. It is used in Australia to regulate floor coverings. The requirements are set out in BCA
Specification C1.10a, providing CRF values for floor coverings based on Class of building, the location within the building (general use or use in fire isolated exits) and whether or not the building is sprinkler protected or not. CRF is measured in kW/m2.

>2.2 and <4.5

Critical Radiance Flux - Higher: This measures the radiant (heat) energy required to sustain burning. It is used in Australia to regulate floor coverings. The requirements are set out in BCA
Specification C1.10a, providing CRF values for floor coverings based on Class of building, the location within the building (general use or use in fire isolated exits) and whether or not the building is sprinkler protected or not. CRF is measured in kW/m2.

≥4.5

Smoke Development Rate: This is the speed at which smoke increases as determined by testing flooring materials in accordance with AS ISO 9239.1. The rate is expressed in terms of percent/minutes. For buildings not protected with a sprinkler system, a maximum smoke development rate of 750 percent/minute applies.

<750
1 - non-combustible 2 - reasonably non-combustible 3 - slightly combustible 4 - combustible

Fire Properties Group
Number:

Average Specific Extinction Area: This value is determined by the volume of smoke measured over the mass loss of the tested sample per test carried out in accordance with ‘Cone Calorimeter Test’ AS/NZS 3837. It is measured in units of m2/kg.

<250

Bushfire Resistance: Naturally bushfire-resisting timbers are those with inherent bushfire-resisting properties. Some species have been tested and a number are in the process of being tested and are measured by Bushfire Attack level (BAL).
BAL -12.5: Ember attack,
BAL – 19: Increasing levels of ember attack and burning debris ignited by windborne embers together with increasing heat flux between 12.5 and 19 kWm3,
BAL – 29: Increasing levels of ember attack and burning debris ignited by windborne embers together with increasing heat flux between 19 and 29 kWm3.

BAL 12.5 and 19 – All AS3959 required applications
Appearance

New England blackbutt has an even texture. The grain is generally straight, making it appealing for interior use applications such as flooring and joinery. The heartwood is pale brown, while the sapwood is much paler in appearance at about 25 - 75 mm wide. Small gum veins are also usually visible.

Common Applications

New England blackbutt is used mainly for general construction applications. In New South Wales and southern Queensland it is very popular for timber framing but is also used for flooring and joinery.

Workability

Care needs to be taken when drying New England blackbutt as it is prone to slight collapse.

It can be stained, painted or polished but there can be issues with painting because of its tendency to surface check. The high extractives of mature wood can cause problems with some adhesives. These extractives can also cause staining on painted surfaces after exposure to the weather.

New England blackbutt machines well but is only fair for steam bending.

Origin of timber
NSW
Readily Available
NSW
New England blackbutt grows in the coastal ranges of New South Wales and the tablelands of northern New South Wales and southern Queensland. It is generally readily available in these areas. Suppliers can provide information on availability in other parts of Australia.
Source of timber
Native Forest
a kitchen with wooden cabinets and a countertop

Joinery

Timber joinery offers a classic, stylish touch to any interior or exterior space.
a house under construction with a roof

Framing

Since people began building simple shelters, wooden framing has played an important role in shaping structures of many kinds. One of the most popular types of wooden framing is known as lightweight timber construction.
a room with benches and paintings on the wall

Flooring

The warmth, strength and natural beauty of timber flooring is enduringly popular in a wide variety of domestic, commercial and industrial applications.

Are you looking for a supplier?

Start Your Search

Social Media Feeds